| ALLOY1 | CASTABILITY | PRESSURE TIGHTNESS |
RESISTANCE TO HOT CRACKING | SOLIDI-FICATION SHRINKAGE |
CORROSION RESISTANCE |
MACHINE- ABILITY |
POLISH- ABILITY |
ELECTRO- PLATING |
ANODIZING (APPEAR- ANCE) |
CHEMICAL OXIDE (PROTECTION) |
STRENGTH AT ELEVATED TEMP |
WELD- ABILITY |
BRAZ- ABILITY |
| 308.1 308.0 |
B |
B | B | B | C | C | C | B | D | NO | C | B | NO |
| 319.1 319.0 |
B+ | B+ | B+ | C | C | C | C | B | D | YES | C | B | NO |
| A319.1 A319.0 |
B | B- | C | B- | C | C | C | B | C | YES | C | B | NO |
| Sr 319.1 Sr 319.0 |
B+ | A | B+ | B | C | B | C | B | D | YES | C | B | NO |
| 332.1 332.0 |
A | B | A | B | C | C | D | C | E | YES | C | B | NO |
| 333.1 333.0 |
A | B+ | B | B | C | B | C | B | D | YES | C | B | NO |
| 336.1 336.0 |
A | B | A | C | C | D | E | D | E | YES | B | B | NO |
| 355.1 355.0 |
B | A | A | B | C | C | C | B | D | YES | B | B | NO |
| C355.2 C355.0 |
B | A | A | B | C | C | C | B | D | YES | B | B | NO |
| 356.1 356.0 |
B | A | A | A | B | C | C | A | D | YES | C | B | NO |
| A356.2 A356.0 |
B | A | A | A | B | C | C | A | D | YES | C | B | NO |
| A443.1 A443.0 |
A | A | A | B | B | E | D | B | D | YES | D | A | LTD. |
| 850.1 850.0 |
E | E | E | E | C | A | A | E | D | YES | E | E | NO |
| 852.1 852.0 |
E | E | E | E | C | A | A | E | D | YES | E | E | NO |
- Aluminum Association Alloy Designations, Janurary, 1989 and ANSI, 1989